Electrical Properties of Metals
Electrical resistivity and conductivity are reciprocal material properties. Their values change with composition, processing and temperature.
A sourced metal reference
| Grade | Conductivity | Derived resistivity | Source condition |
|---|---|---|---|
| Copper C11000 (ETP) | 58 MS/m | ≈ 1.724 × 10⁻⁸ Ω·m | Copper Development Association design guide; nominal physical values. Conductivity is a rounded guide value, not an acceptance limit. CDA guide |
The resistivity is calculated as 1 / (58 × 10⁶). It inherits the rounding and applicability of the source conductivity. This is not a minimum conductivity requirement for every product sold under that designation.
Sourced resistivity at a stated temperature
Resistivity ρ is in ohm metres. Conductivity is calculated as 1/ρ and shown in MS/m, so it carries the same uncertainty and temperature as the source value. A range means the source printed a range; neither end is a minimum or acceptance limit. Rows from datasheets that give no temperature say so. Pure-element values from the HyperPhysics table are for 20 °C. Commercial alloys vary with composition and temper.
| Material, grade | Resistivity Ω·m | Conductivity MS/m (calculated, 1/ρ) | Temperature |
|---|---|---|---|
| Aluminium 6061 6061-T6 extrusions, BS EN 755-2 | 4 × 10−8 1 | 25 | Temperature not stated by the source |
| Stainless steel 304 1.4301 (304) bar and section, EN 10088-3 | 7.2 × 10−7 2 | 1.39 | Temperature not stated by the source |
| Stainless steel 316 1.4401 (316) bar and section, EN 10088-3 | 7.4 × 10−7 3 | 1.35 | Temperature not stated by the source |
| Brass CW614N CW614N rod, EN 12164 | 6.2 × 10−8 4 | 16.1 | Temperature not stated by the source |
| Copper CW004A CW004A (pure copper) sheet, plate and bar | 1.71 × 10−8 5 | 58.5 | Temperature not stated by the source |
| Silver Element, purity not stated | 1.59 × 10−8 6 | 62.9 | 20 °C |
| Aluminium (pure) Element, purity not stated | 2.65 × 10−8 6 | 37.7 | 20 °C |
| Tungsten Element, purity not stated | 5.6 × 10−8 6 | 17.9 | 20 °C |
| Iron (pure) Element, purity not stated | 9.71 × 10−8 6 | 10.3 | 20 °C |
| Lead Element, purity not stated | 2.2 × 10−7 6 | 4.55 | 20 °C |
| Carbon steel EN C45 (1.0503), Ovako material data sheet | 2 × 10−7 to 2.5 × 10−7 7 | 4 to 5 | "Ambient temperature"; range as printed |
| Aluminium 7075 7075-T6, NASA Materials Data Handbook | 5.2 × 10−8 8 | 19.2 | 20 °C |
| Titanium Ti-6Al-4V Grade 5, Upmet datasheet | 1.71 × 10−6 9 | 0.585 | 68 °F (20 °C) |
| Gold Foil (Goodfellow) | 2.2 × 10−8 10 | 45.5 | 20 °C |
| Nickel Nickel 200/201, ATI datasheet | 8.5 × 10−8 11 | 11.8 | 27 °C (80 °F), not 20 °C; one table for both ATI 200 and ATI 201 |
- Aalco datasheet, Al 6061-T6 (accessed 2026-11-24)
- Aalco datasheet, 1.4301 (304) (accessed 2026-11-24)
- Aalco datasheet, 1.4401 (316) (accessed 2026-11-24)
- Aalco datasheet, brass CW614N (accessed 2026-11-24)
- Aalco datasheet, copper CW004A (accessed 2026-11-24)
- HyperPhysics resistivity table (accessed 2026-11-24)
- Ovako Steel Navigator, C45 (accessed 2026-11-24)
- NASA Materials Data Handbook, aluminium alloy 7075 (accessed 2026-11-24)
- Upmet Ti-6Al-4V datasheet (accessed 2026-11-24)
- Goodfellow gold foil (accessed 2026-11-24)
- ATI Nickel 200/201 datasheet (accessed 2026-11-24)
Nickel is quoted at 27 °C because that is the temperature in the source table. Carbon steel is shown as the range printed by the source.
From a material value to resistance
For a uniform conductor, R = ρL/A. A 1 m conductor with 1 mm² area and the reference resistivity above gives approximately 0.01724 Ω. Real connections add contact resistance; AC operation can introduce skin and proximity effects.
Comparing other metals
Use the specific alloy data sheet, temperature and condition. Pure-element values do not stand in for a commercial steel or aluminium alloy. Keep conductivity, resistivity and total component resistance in separate columns.
Convert resistivity units →Sources & further reading
- live.copper.org pdf / a1360.pdf
- nist.gov pml / special-publication-811
- aalco.co.uk datasheets / Aluminium-Alloy-6061-T6-Extrusions_145.ashx
- aalco.co.uk datasheets / Stainless-Steel-14301-304-Bar-and-Section_34.ashx
- aalco.co.uk datasheets / Stainless-Steel-14401-316-Bar-and-Section_37.ashx
- aalco.co.uk datasheets / Copper-and-Copper-Alloys-CW614N-Brass-Rod_31.ashx
- aalco.co.uk datasheets / Copper-and-Copper-Alloys-CW004A-Sheet-Plate-and-Bar_32.ashx
- hyperphysics.phy-astr.gsu.edu Tables / rstiv.html
- steelnavigator.ovako.com c45 / pdf
- ntrs.nasa.gov downloads / 19720022809.pdf
- upmet.com datasheet / ti-6al-4v-datasheet.pdf
- goodfellow.com usa / gold-foil-1000016296
- atimaterials.com nickel-based / ati_200_201_tds_en1_v1.pdf